Pressed Wood in the Preparation of Friction Parts,
Abstract
Improved antifriction properties are ensured by 70-75% in weight of wood and 25-30% in weight of fluoroplastic filler. The pore filling with the plastic is carried out in vacuum with or without the aid of ultrasonic vibrations. This is followed by drying to a humidity content of 18 to 20%, pressing under 200-250 Kg/sq cm and at a temperature of 105-110C with subsequent treatment at 155-165C. (Author)